Polyvinyl alcohol fiber (PVAF) is an ideal environment-friendly cement reinforcement material successfully developed by our company recently. Because of its unique molecular structure, it has a good affinity with cement and suitable alkali and weather resistance. Effectively prevent and inhibit the formation and development of cracks, improve concrete’s bending, impact, and cracking strength, and improve concrete’s impermeability, impact resistance, and earthquake resistance. It can be widely used in walls, roofs, floors and roads, bridges, tunnels, and slope reinforcement of industrial and civil buildings. Currently, in cement concrete engineering, due to the unique properties of PVA fiber, it has broad development prospects in engineering and construction applications, and it is an ideal new product that can completely replace asbestos.

纤维直径

fibre diameter

15μm±3

 

断裂强度

breaking strength

≥1200MPa

 

弹性模量

elasticity modulus

≥35GPa

 

断裂伸度

breaking elongation

6-11%

 

耐热水性

Hot Water Resistance

≥98℃

 

干热软化点

softening point in hot air

≥216℃

 

长度

length

6mm、12mm

 

Performance
  1. High strength and low elongation: superior mechanical properties.
  2. Acidity and alkalinity: The strength loss is low in a long-term acid-base environment.
  3. Corrosion resistance: The fiber is buried underground for a long time without mold, decay, or insects.
  4. Dispersion: The fiber does not stick together, has good water dispersibility, and has a good affinity with cement.

Function

1.Anti-crack and anti-seepage: The fibers are randomly distributed in the concrete (mortar), which can effectively prevent the occurrence and development of cracks and improve the ability of waterproof and anti-seepage.

Usage of PVA fiber and PA (nylon) fiber

纤维种类

Fiber type

纤维掺入量(g/m³)

Fiber content

裂缝减少率%

crack reduction rate

PA(尼龙)

PA (nylon)

900  43

 

PVA混凝土/砂浆专用纤维

PVA concrete/mortar special fiber

900  86

 

 

2.Shock and earthquake resistance: Effectively absorb impact energy and improve earthquake resistance.

Cement board reinforcement test performance comparison table

品种type

 

纤维性能fiber property

 

水泥板性能Cement board property

 

水泥板配方

Cement board formula

纤度(d)

dtex

强度(kg/cm²)

strength

伸度 (%)

elongation

杨氏模量(kg/cm²)

Young modulus

弯曲强度      (kg/cm²)

bending strength

韧性(面积比)

Toughness

(area ratio)

冲击强度(kg/cm²)

Impact strength

裂缝(天)

Crack(day)

PVA混凝土

PVA Concrete

 

2.4 15.2 6.0 3685 378 42 4.9 30以上

More than 30 days

纤维:水泥:硅砂

Fiber: Cement: Silica sand

砂浆专用纤维

Special fiber for mortar

 

2.4 14.4 6.8 3127 356 38 4.3 30以上

More than 30 days

0.003 :1:2

 

石 棉

asbestos

  240 1 2.3 1 石棉(湿):泥浆:水泥

Asbestos (wet): Mud: Cement

15  : 3 : 82

 

 

3.Improve the frost resistance and fatigue resistance of concrete.

4.Increase toughness: improve the brittleness of concrete,impact and bending resistance.

 Application scope
  1. Large-volume concrete pouring and guardrails, damsand parking lots.
  2. Make concrete components, platesand light wall panels to replace asbestos and make asbestos cement products.
  3. Shotcrete for tunnels, minesand culverts.
  4. Make light wall panels, GRC boards, insulation boards, and other building materials.

Usage

  1. The original proportion of concrete remains unchanged, and the fibers are accurately weighed according to the designed addition amount and the amount of concrete mixed each time.
  2. After the gravel material is ready, add the fiber, the aggregate, and water to the mixer, then stir.
  3. After the mixing is completed, take random samples. The concrete can be used if the fibers have been evenly dispersed into monofilaments. If there are still bundles of fibers, prolong the mixing time for 30-60 seconds, and then it can be used.
  4. Fiber-added concrete’s construction and maintenance process is identical to ordinary concrete’s.
  5. Product dosage: Generally speaking, for plain slurry or mortar, fiber-reinforced cement slabs, and corrugated tiles, the dosage range is 0.6-1kg/m³, and the standard dosage is 0.6kg/m³; for concrete, the dosage range is 0.6-1.9 kg/m³, the usual amount is 0.9kg/m³.